ASTM A387 is a specification for chromium-molybdenum alloy steel plate for welded boilers and pressure vessels in elevated-temperature service. Grade 5 contains about 5% chromium and 0.5% molybdenum, which improve oxidation resistance, creep strength and sulfidation resistance.
ASTM A387 Grade 5 alloy steel plate is a 5Cr-0.5Mo chrome-moly plate for hot, corrosive process duty. Conquest Steel & Alloys, a Mumbai-based stockist, supplier and exporter of alloy steel plates since 2008, supplies ASTM A387 / ASME SA387 plate on enquiry. Refinery, petrochemical, power and chemical buyers use it for pressure vessels, heat exchangers and boiler parts.
ASTM A387 Grade 5 is a chromium-molybdenum alloy steel plate with about 5% chromium and 0.5% molybdenum. Engineers also call it 5Cr-½Mo or chrome moly plate. The ASME twin is SA387 Grade 5, and buyers often search for it as “ASTM 387 Grade 5”, though the correct designation is A387.
Chromium builds oxidation and sulfidation resistance, and molybdenum builds creep strength. Together they let the plate hold up in hot, sulphur-bearing service where carbon steel and carbon-molybdenum steel wear out faster.
The grade comes in two classes. Class 1 is the lower-strength condition, and Class 2 is the higher-strength condition. Both use the same chemistry and differ in heat treatment and mechanical properties.
Many buyers search for “A387 Grade 5 plate manufacturers in Mumbai”. Conquest is a stockist and supplier, not a mill. We source plates from mills that follow international plate production guidelines, then stock, cut and dispatch them from our Mumbai-region yards.
The main features are oxidation and sulfidation resistance, creep strength and weldability with the right procedure.
1. Oxidation and Sulfidation Resistance - About 5% chromium forms a protective oxide film on hot surfaces. That gives Grade 5 better scaling and sulphur-attack resistance than lower-chromium grades. Your engineer should still check the service temperature and sulphur level.
2. Creep Strength at Temperature - Molybdenum raises creep strength, so the plate keeps its load-bearing ability in long hot service. Design codes set the allowable stress at each temperature.
3. Two Strength Classes - Class 1 offers 415 to 585 MPa tensile strength. Class 2 offers 515 to 690 MPa. Pick the class your design stress needs.
4. Weldable with Controlled Procedure - Chrome-moly steels weld well when fabricators follow a qualified procedure. Expect preheat, controlled interpass temperature and post-weld heat treatment, as the code requires.
5. Clean, Heat-Treated Plate - Plate ships annealed, normalised and tempered, or quenched and tempered, depending on the class. Our cutting to size service reduces scrap and handling.
A design note: 5Cr-0.5Mo is a low-alloy steel, not a stainless steel. It does not resist wet corrosion or chloride attack like stainless. Also review temper embrittlement risk if the plate will spend long periods in the mid-temperature range.
ASTM A387 Grade 5 is most often cross-referenced to EN 10028-2 X12CrMo5 and GOST 15Kh5M. The table shows the usual equivalent designations. Each is a reference only, because chemistry and heat treatment limits differ between standards.
| Region | Standard | Equivalent designation |
|---|---|---|
| USA (ASTM) | ASTM A387 | Grade 5, Class 1 / Class 2 |
| USA (ASME) | ASME SA387 | Grade 5, Class 1 / Class 2 |
| USA (UNS) | UNS | K41545 |
| EU | EN 10028-2 | X12CrMo5 (1.7362) |
| Russia / CIS | GOST | 15Kh5M |
Confirm the match on the mill test certificate. Substituting a grade without engineering approval can invalidate a design basis.
ASME SA387 Grade 5 matches ASTM A387 Grade 5 in grade and chemistry. The ASME edition carries the Section II stamp that boiler and pressure vessel codes require.
| Item | ASTM edition | ASME edition |
|---|---|---|
| Specification | ASTM A387 | ASME SA387 |
| Grade | Grade 5 | Grade 5 |
| Class 1 tensile | 415 to 585 MPa | 415 to 585 MPa |
| Class 2 tensile | 515 to 690 MPa | 515 to 690 MPa |
| Typical use | General plate supply | Code-stamped pressure equipment |
For pressure equipment, confirm whether your code requires the ASME SA edition or accepts the ASTM edition.
Grade 5 combines 4.00 to 6.00% chromium with 0.45 to 0.65% molybdenum. Heat analysis and test results on the mill test certificate govern every order.
| Element | Content (%) |
|---|---|
| Carbon (C) | 0.15 max |
| Manganese (Mn) | 0.30 to 0.60 |
| Phosphorus (P) | 0.025 max |
| Sulphur (S) | 0.025 max |
| Silicon (Si) | 0.50 max |
| Chromium (Cr) | 4.00 to 6.00 |
| Molybdenum (Mo) | 0.45 to 0.65 |
| Property | Class 1 | Class 2 |
|---|---|---|
| Tensile strength | 415 to 585 MPa | 515 to 690 MPa |
| Yield strength (min) | 205 MPa | 310 MPa |
| Elongation in 50 mm (min) | 22% | 22% |
| Elongation in 200 mm (min) | 18% | 18% |
Class 2 delivers about 100 MPa more tensile strength and 105 MPa more yield strength than Class 1. Both classes share the same 5Cr-0.5Mo chemistry, so heat treatment drives the difference.
| Class | Tensile strength (MPa) | Yield strength, min (MPa) | Typical fit |
|---|---|---|---|
| Class 1 | 415 to 585 | 205 | Moderate stresses; easier fabrication |
| Class 2 | 515 to 690 | 310 | Higher design stress; thinner sections |
| Grade | Nominal chemistry | Common positioning |
|---|---|---|
| A387 Grade 11 | 1.25Cr-0.5Mo | General elevated-temperature vessels |
| A387 Grade 22 | 2.25Cr-1Mo | Creep strength in hot service |
| A387 Grade 5 | 5Cr-0.5Mo | Oxidation and sulfidation resistance |
| A387 Grade 9 | 9Cr-1Mo | Higher-temperature oxidation resistance |
Choose the grade by temperature, sulphur content and design code, and choose the class by design stress.
ASTM A387 Grade 5 plate serves industries that run heat, pressure and sulphur-bearing fluids together. Typical uses include:
Match each use to its service. Wet, chloride or acidic duty needs a separate material review.
Conquest arranges A387 plate in several grades and many related designations. Our team handles enquiries for:
We also supply related carbon-molybdenum plate such as ASTM A204. Share your grade, class and thickness so we can confirm availability.
Indicative A387 Grade 5 plate pricing in Mumbai runs roughly ₹175 to ₹250 per kg (₹1,75,000 to ₹2,50,000 per tonne). Every figure is indicative and depends on class, thickness, quantity, cutting and market rates. None is a fixed quote.
| Product form | Grade | Indicative range (₹ per kg) | Indicative range (₹ per tonne) |
|---|---|---|---|
| Alloy steel plate | ASTM A387 Grade 5, Class 1 | 175 to 250 | 1,75,000 to 2,50,000 |
| Alloy steel plate | ASTM A387 Grade 5, Class 2 | 175 to 250 | 1,75,000 to 2,50,000 |
A387 is a plate specification, so the table covers plate only. For coil, pipe or tube in related alloy grades, send an enquiry.
Conquest Steel & Alloys has supplied steel plates from Mumbai since 2008. It draws on 30 years of promoter and partner experience in steel sourcing, stocking and supply chain. Buyers know us as a stockist, supplier and exporter of alloy steel plates across India.
Our footprint grew step by step:
What this means for your order:
Our plan is to add a dedicated logistics team to cut delivery costs for customers.
Conquest supplies alloy steel plate across India and to export markets.
All exports are subject to applicable trade rules.
ASTM A387 Grade 5 is commonly cross-referenced to ASME SA387 Grade 5, EN 10028-2 X12CrMo5 (1.7362) and GOST 15Kh5M. All describe a 5% chromium, 0.5% molybdenum steel, but limits and heat treatment differ. Confirm the match against your design code and the mill test certificate before ordering.
Class 1 and Class 2 share the same chemistry and differ in heat treatment and strength. Class 1 offers 415 to 585 MPa tensile and 205 MPa minimum yield. Class 2 offers 515 to 690 MPa tensile and 310 MPa minimum yield. Class 2 suits higher design stresses.
ASTM A387 covers chromium-molybdenum plate in grades 2, 11, 12, 21, 22, 5, 9 and 91, most supplied in Class 1 and Class 2. Chromium content rises from about 0.5% in Grade 2 to 9% in Grades 9 and 91, improving oxidation and creep resistance at higher temperatures.
Grade 5 carries about 5% chromium and 0.5% molybdenum, which favours oxidation and sulfidation resistance. Grade 22 carries about 2.25% chromium and 1% molybdenum, which favours creep strength. Refineries and chemical plants pick between them based on temperature, sulphur content and design code.
ASTM A387 Grade 5 alloy steel plate gives fabricators a proven chrome-moly option for pressure equipment that faces heat and sulphur-bearing fluids. Its 5% chromium builds oxidation and sulfidation resistance, its molybdenum adds creep strength, and its two classes let you match the plate to your design stress. Choosing the right class, 1 or 2, keeps your design code, cost and fabrication in balance.
Choosing the right supplier matters as much as choosing the right grade. Conquest Steel & Alloys has served steel buyers from Mumbai since 2008, backed by 30 years of promoter and partner experience in steel sourcing, stocking and supply chain. We stock plates at our Kalamboli and Taloja yards, cut to size on request, run ultrasonic testing in-house and arrange documentation for quality records.
Before you order, send us your drawing or cutting list, the required grade and class, thickness, width and length, the quantity, and your delivery location. State whether you need the mill test certificate with the dispatch and which code, ASTM A387 or ASME SA387, your design follows. We will confirm availability and share an indicative price, then convert it into a formal quote once the details are final.
Ready to move? Request a quote today. Call our Mumbai sales team on +91 22 23894572 (Monday to Saturday, 10 am to 6 pm) or email csa@csteel.in with your requirement. Our team will respond with stock status, lead time and pricing for ASTM A387 Grade 5 alloy steel plate . Whether you need one plate or a full project lot, we are ready to help.
| India Price : | Min- 150 INR Per Kg / Max- 200 INR Per Kg |
|---|---|
| USD Price : | Min- 1.71 USD Per Kg / Max- 2.28 USD Per Kg |
| Grade : | ASTM A387 GR.5 CL.1 |
| Standard : | ASTM A387 / ASME SA387 |
| Thickness : | 6 mm to 150 mm |
| Width : | Up to 3000 mm |
| Length : | Up to 12000 mm |
| Elongation : | 20% min |
| Tensile Strength : | 415 – 585 MPA |
| Yield Strength : | Min. 205 MPA |